Guyana is hot, wet and humid for most of the year. That’s hard on people, and it’s hard on welding consumables too. Moisture is one of the main sources of hydrogen in a weld, and hydrogen is one of the main causes of cracking in carbon and low-alloy steel welds. It’s one of the first things our welding inspectors check on any job here.
Why moisture causes problems
Water in an electrode coating or a flux breaks down in the arc and releases hydrogen into the weld pool. Some of it stays trapped as the weld cools. In a hard heat-affected zone with some residual stress, that hydrogen can cause cracks – sometimes hours or days after welding, when the weld has already passed visual inspection.
Low-hydrogen electrodes need looking after
Low-hydrogen electrodes such as E7018 are designed to keep hydrogen low, but only if they stay dry. Once a sealed tin is opened, the electrodes start absorbing moisture from the air. Manufacturers and codes set limits on how long they can be exposed. In a humid climate that time runs out quickly.
- Store opened electrodes in a heated holding oven at the temperature the manufacturer recommends.
- Issue them to welders in a heated quiver, not a pocket or an open box.
- Return unused electrodes to the oven, or re-bake them following the manufacturer’s instructions where re-baking is allowed.
- Throw away electrodes that have got wet. Re-baking doesn’t fix damaged coatings.
Flux and wire need care too
Submerged arc flux should be kept sealed or stored in a heated hopper, and re-dried if it’s been exposed. Flux-cored wire is less sensitive than stick electrodes but still shouldn’t sit out in the rain or in a damp container overnight. Rust on solid wire causes porosity and feeding problems.
Don’t forget the steel
Morning condensation and rain on the joint itself bring moisture into the weld just as surely as a wet electrode. Preheat – even a modest one where it isn’t strictly required – drives off surface moisture. Tents and shelters help on site.
What our inspectors look for
Oven temperatures and records, quivers in use, open tins on benches, electrodes left in the sun or rain, and joints that are visibly wet. These are small things. Fixing them costs very little compared with finding delayed cracking in a finished structure.